Bosses are one of the most common features in injection molded parts. They look simple: a raised circular structure used for self-tapping screws, threaded inserts, press-fit plugs, or locating pins.
But many assembly line problems — stripped screws, cracked bosses, insufficient pull-out strength — start at the design stage. This article doesn't cover "what is a boss." It covers a few details that are easy to overlook, and the consequences of ignoring them.
If you're sourcing custom injection molded components, these are the design details worth checking before your mold is cut.
The intersection creates a thick section. That section cools slower, causing sink marks on the opposite surface or voids inside. When a self-tapping screw is driven in, it creates hoop stress. If the screw hits a void, pull-out strength drops.
Connect the boss to the side wall with a rib instead (see Figure 1-1). The rib adds stiffness and gives gas a path to escape during filling. Gas travels from the boss through the rib to the side wall, and vents at the parting line.

Too small — the wall is thin, and hoop stress from the screw can crack it.
Too large — the wall is thick, the interior cools slowly, and voids form. The screw may hit a void instead of solid plastic. The screw feels tight, but pull-out strength is compromised.
For high-modulus plastics, this ratio varies with screw design. Specialty screw manufacturers publish recommended dimensions for different materials.
Taller bosses are harder to fill, pack, and eject. The core pin can deflect under injection pressure, making the wall thickness uneven. The thin side becomes a crack initiation site.
Where the boss meets the main wall: radius = 25% of wall thickness, minimum 0.25mm.
Where the inner wall meets the base: radius = 10% of wall thickness.
Base wall thickness = 75% of main wall.
These radii distribute stress. Without them, stress concentrates at the sharp corner. When the screw is driven in, the crack starts there.

The melt flows around the core pin and meets on the far side. That weld line is a butt weld — the weakest type. When a screw is driven in, hoop stress runs perpendicular to it. The weld line fails first.
Expect weld lines on hollow bosses. Design around them.
Medium and low modulus plastics: forming screws work.
High modulus plastics: cutting screws are required. Forming screws generate too much strain and can crack the boss.
The wrong type leads to cracking, especially in glass-filled resins.
Design Detail | Recommendation |
Boss connection | Rib to side wall — never direct |
Inner diameter | Pitch diameter of screw |
Outer diameter | ~2.5 × inner diameter |
Height | ≤ 2.5 × inner diameter |
Base fillet | 25% of wall thickness (min 0.25mm) |
Inner base fillet | 10% of wall thickness |
Base wall thickness | 75% of main wall |
Top chamfer | 45° |
Outer draft | ≥ 0.5° |
Screw type | Forming for low/medium modulus; cutting for high modulus |