CN Mould & Plastic Limited

Case Study: How We Fixed a Stubborn Gloss Mark on a Textured ABS Part

Table of Content [Hide]

    We recently ran into a stubborn defect while trial-running a new ABS faceplate. Right on the sidewall—a highly visible cosmetic area—we saw distinct glossy marks (see Figure 3-1).

     

    If you’ve ever dealt with gloss variation on a matte surface, turned down the packing pressure, and watched the defect stay exactly in the same place, this case study is for you.

     

    What Are Gloss Marks?

    In the industry, these are often called stress marks. They show up as localized shiny areas that clash with the surrounding matte finish, and for cosmetic parts, they’re a fast track to customer rejection.

     

    The Standard Playbook (And Why It Didn’t Work)

    Normally, gloss marks point to process issues: injection or packing pressure too high, packing time too long, injection speed too low, or mold temperature too low.

     

    Our engineers started with the standard fix. We dropped the injection and packing pressures and ran another shot. The mark lightened up—but it didn’t disappear. More importantly, its location didn’t shift.

     

    Here’s the critical takeaway: If adjusting process parameters only reduces the severity of the mark, but the location stays exactly the same, it’s not a process problem. If you keep tweaking the machine, you’re treating the symptom, not the root cause.

     

    The Clue: Look at the Mold Texture

    We shifted our focus from the injection machine to the tool. This mold uses an etched texture to give the part its uniform matte finish.

     

    When the depth, uniformity, or local condition of the mold texture doesn’t match the plastic’s shrinkage stress during packing, the stress builds up. Once the part demolds, that localized stress shows up as a shiny patch.

     

    In other words, if the gloss mark is in a fixed location on a textured surface, the problem isn’t in your parameters. It’s in the microscopic state of the mold cavity.

     

    The Solution: Re-Etching the Mold

    We pulled the mold and re-processed the texture. The point wasn’t to keep tweaking the injection profile—it was to change the microscopic surface condition of the mold so the light reflection in that stress zone matched the rest of the part.

     

    Once the texture was redone, the stress from shrinkage matched the mold surface properly, and the conditions for the defect were eliminated.

     

    The Verification

    With the mold back on the machine, we ran another trial. The surface gloss was perfectly uniform. The gloss marks were gone.


    case-study-how-we-fixed-a-stubborn-gloss-mark-on-a-textured-abs-part1.jpg

     

    Summary: How to Troubleshoot Gloss Marks on Textured ABS

    1. Try the standard process tweaks first. Lower pressures, raise mold temp, shorten hold time, increase injection speed. See if the mark moves.

     

    2. Stop if it doesn’t move. If adjusting parameters only lightens the mark and the location stays fixed—especially on an etched surface—suspect the mold.

     

    3. Check the texture. Inspect the uniformity of the mold etching. Don’t waste hours on the machine. Re-etching the mold is often the only way to truly eliminate the defect.


    References
    PREV: No information
    #ADVANCED MANUFACTURING
    Discover Other Injection Moulding News
    #SPECIAL
    Recyclable Plastic Material In Normal Life
    08-08
    Recycling plastic is crucial for both the environment and our way of life, according to CN Mould & Plastic Limited. Since 2000, we have been pleased to support a large number of clients with the u...
    Glass Transition Temperature (Tg): Why It Matters for Plastic Part Design
    06-25
    When selecting a plastic material for a specific application, glass transition temperature (Tg) is one of the most important properties to consider.The transition from a glassy state to a rubbery stat...